sales@jitaivalve.com    +86-577-86613556
Cont

Have any Questions?

+86-577-86613556

Jul 16, 2021

Causes For Rusting Of Butterfly Valves During Use

_20210619164538_




Stainless steel butterfly valves will inevitably rust during use. It is very important to find out what causes the stainless steel butterfly valve to rust. Through the analysis of the material structure of the butterfly valve, heat treatment test, SEM and other test panels. Because the carbides along the grain boundaries in the valve material precipitate to form a sub-marking zone, this is the reason for the corrosion of the stainless steel butterfly valve.

 

The stainless steel butterfly valve made of CF8M is corroded during use. Austenitic stainless steel after normal heat treatment, the tissue should be at room temperature Austria 's body, good corrosion resistance. In order to analyze the cause of the rust of the butterfly valve, a sample was taken on it for analysis .

1 Test method

Sampling for chemical composition analysis (judging whether it meets the standard requirements), metallographic structure inspection, heat treatment process test and SEM analysis.

2 Test results and analysis

"Table 1 " Chemical   composition analysis results /%

Ingredients

C

Si

Mn

P

S

Cr

Ni

Mo

CF8M

0.08

1.5

1.5

0.04

0.04

18~21

9~12

2~3

Butterfly valve

0.10

0.60

0.61

0.024

0.009

18.05

9.71

1.45


2.1 Chemical composition

The chemical composition analysis results and standard composition are shown in "Table 1 ".

2.2 Metallographic analysis

Metallographic specimens were cut from the rusted butterfly valve. After grinding and polishing, they were corroded with an aqueous solution of ferric chloride and observed and analyzed on the Neophot-32 metallographic microscope. The metallographic structure is composed of austenite and another Species of precipitate composition. Theoretically speaking, austenitic stainless steel should get a uniform austenitic structure after normal heat treatment. There are two kinds of judgments about the structure of another precipitate that appears in the organization: one is the σ phase, and the other is the carbide. σ phase and carbide formation conditions are different, but they all have a common feature, that is, the sensitivity of austenitic stainless steel to intergranular corrosion.

First, the variegation method is used to identify the σ phase. Using alkaline aqueous solution of red blood salt ( 10g of red blood salt + 10g of potassium hydroxide + 100ml of water ), after the sample is boiled in this reagent for 2 to 4 minutes , the ferrite is yellow, the carbides are corroded, and the austenite is Bright color, σ phase changes from brown to black. The sample cut from the butterfly valve was boiled in an alkaline red blood saline solution for 4 minutes by the above method , and then observed under a microscope, the precipitates maintained their original morphology, and no significant changes were found. Therefore, it was decided to use the heat treatment method to further test the face analysis.

2.3 Heat treatment test analysis

The sigma phase is an intermetallic compound with approximately the same atomic ratio of iron to chromium. Chemical composition, ferrite, cold deformation, and temperature change all affect the formation of σ phase to varying degrees . The staining method was used to test, and the precipitation phase change was not obvious under the microscope, so the heat treatment method was used to identify the σ phase. According to relevant information, σ phase is usually formed during long-term aging at 500~800 ℃ . This is because aging at higher temperatures is conducive to the diffusion of chromium. Heating the σ phase at a higher temperature will begin to dissolve, and the dissolution must be at least 920 ℃ or more. Heating at a stable temperature higher than the σ phase can eliminate it. Although it takes a long time to form the σ phase, the elimination of the σ phase generally requires only a short heating time. According to this theory, a heat treatment process was developed to observe whether the precipitated phase in the structure can be eliminated. The sample cut from the butterfly valve is heated to 940 ℃ , kept for 30 minutes , and then observed and analyzed on a Neophot-32 metallurgical microscope. After the heat treatment, the precipitated phase in the sample is not eliminated and the original morphology is maintained, which proves that the precipitated phase in the structure may not be a sigma phase.

2.4 SEM analysis

Sometimes the sigma phase in steel cannot be distinguished by any dyeing method. It can be identified by SEM analysis method. Because it is known that the σ phase is a compound of iron and chromium, with a chromium content of 42% to 48% , the constituent elements and their contents of the unknown phase are measured by EDS qualitative and quantitative analysis, so as to determine the unknown phase.

The results of micro-area quantitative analysis of the matrix and precipitates are shown in "Table 2 ".

"Table 2 " EDS quantitative   analysis results /%

Ingredients

Fe

Cr

Ni

Mo

Si

Mn

Matrix

70.463

16.365

10.211

1.239

0.466

1.257

Precipitated   phase

56.908

33.629

3.681

4.835

0.040

0.907

EDS analysis showed that the amount of chromium containing precipitate was 33.6% , significantly higher than in the matrix Cr content of 16.3% , while σ amount of chromium-containing phase is 42% -48% , thus denying precipitates as σ phase. Based on the results of the dyeing test and the heat treatment test, it is believed that the precipitated phase in the structure of the stainless steel butterfly valve is not the σ phase. Observed by SEM, the precipitated phase is a kind of eutectic structure, which is mainly chromium carbide.

The stainless steel butterfly valve is made of nickel-chromium austenitic stainless steel, which is generally used in a solid solution state. At room temperature, its structure is austenitic. Austenitic stainless steel has good corrosion resistance in a wide range of corrosive media, especially in the atmosphere. The reasons for the corrosion of stainless steel butterfly valves are as follows:

① Based on the results of the above tests, it can be determined that the precipitated phase in the butterfly valve material structure is not the σ phase, so the rust phenomenon of the butterfly valve is not caused by the σ phase.

② Through SEM observation, it is confirmed that the precipitated phase in the structure of the butterfly valve is mainly chromium carbide, and this eutectic structure is distributed along the grain boundary. The EDS analysis results show that the chromium content of this carbide distributed on the grain boundary is significantly higher than that of the matrix. This carbide is of type M 23C6 . With the precipitation of carbides and no chromium diffusion supplementation, chromium carbides precipitate along the austenite grain boundaries, forming a chromium-depleted zone around the carbides, so that the austenitic stainless steel grain boundaries are easily corroded. Therefore, the carbide precipitated along the grain boundary is the main cause of the rust of the butterfly valve.

③For the austenitic stainless steel after solution treatment, because most of the carbides are dissolved when heated at high temperature, the austenite is saturated with a large amount of carbon and chromium , and the austenite is fixed due to the subsequent rapid cooling, so that the material has a lot of The corrosion resistance of the quotient. Therefore, the heat treatment process should be strictly controlled. During the solution treatment, the workpiece is heated to high retreat to fully dissolve the carbide, and then rapidly cooled to obtain a uniform Austenite structure. After solution treatment, if slow cooling is used, chromium carbide will precipitate along the grain boundary during the cooling process, which will result in a decrease in the corrosion resistance of the material.


Send Inquiry